锰钴镍氧浸没式探测器制备及性能
作者:
作者单位:

中国科学院上海技术物理研究所 红外物理国家重点实验室,中国科学院上海技术物理研究所 红外物理国家重点实验室,中国科学院上海技术物理研究所 红外物理国家重点实验室,中国科学院上海技术物理研究所 红外物理国家重点实验室,中国科学院上海技术物理研究所 红外物理国家重点实验室

作者简介:

通讯作者:

中图分类号:

基金项目:

国家自然科学基金:11204336, 61274138, 61275111 及 11304336, 上海市基金:12ZR1452200, 上海技术物理所创新专项:Q-ZY-86。National Natural Science Foundation of China (11204336, 61274138, 61275111 and 11304336), Shanghai Project (12ZR1452200), Innovation project of Shanghai Institute of Technical Physics (Q-ZY-86).


Fabrication and performance of Mn-Co-Ni-O thin film infrared detector
Author:
Affiliation:

National Laboratory for Infrared Physics,Shanghai Institute of Technical Physics,Chinese Academy of Sciences,National Laboratory for Infrared Physics,Shanghai Institute of Technical Physics,Chinese Academy of Sciences,National Laboratory for Infrared Physics,Shanghai Institute of Technical Physics,Chinese Academy of Sciences,National Laboratory for Infrared Physics,Shanghai Institute of Technical Physics,Chinese Academy of Sciences,National Laboratory for Infrared Physics,Shanghai Institute of Technical Physics,Chinese Academy of Sciences

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    基于化学溶液法制备了尖晶石结构氧化物锰钴镍氧Mn1.56Co0.96Ni0.48O4(MCNO)薄膜材料, 研究了其电学性质及红外器件的探测性能, 包括器件的响应率, 时间常数和探测率.制作了厚度为8μm的MCNO薄膜及红外热敏探测器件, 测量了材料的阻值-温度曲线.制作了基于半球形锗透镜的浸没式MCNO薄膜探测器, 具有时间常数较小(~18ms), 响应率高(~4.4×103V/W)和探测率高(~5×108cm·Hz0.5/W)的优点.

    Abstract:

    Spinel oxide Mn-Co-Ni-O (MCNO) thin films were prepared by using a chemical solution deposition method (CSD). The electrical property and device performance based on MCNO thin films were investigated, including the responsivity (RV), noise spectra and the detectivity (D*). MCNO thin film with a thickness of 8μm was prepared and their sheet resistance versus temperature curves are measured. The optical immersed MCNO infrared detector based on Germanium lens was fabricated, and it possesses the advantages of relatively small time constant (~18ms), high responsivity (~4.4×103V/W) and high detectivity (~5×108cm·Hz0.5/W).

    参考文献
    相似文献
    引证文献
引用本文

周 炜,欧阳程,吴 敬,高艳卿,黄志明.锰钴镍氧浸没式探测器制备及性能[J].红外与毫米波学报,2015,34(2):161~165]. ZHOU Wei, OU Yang-Cheng, WU Jing, GAO Yan-Qing, HUANG Zhi-Ming. Fabrication and performance of Mn-Co-Ni-O thin film infrared detector[J]. J. Infrared Millim. Waves,2015,34(2):161~165.]

复制
分享
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2014-01-13
  • 最后修改日期:2015-02-06
  • 录用日期:2014-01-24
  • 在线发布日期: 2015-05-18
  • 出版日期:
文章二维码